June 2026: We are continuing a major code rewrite. Please contact us if you find issues. Thank you.
| Oxide | Analysis | Formula | Tolerance |
|---|---|---|---|
| CaO | 0.10% | - | |
| K2O | 0.22% | 0.01 | |
| MgO | 0.05% | - | |
| Na2O | 0.02% | - | |
| TiO2 | 1.78% | 0.06 | |
| Al2O3 | 37.78% | 1.00 | |
| SiO2 | 45.92% | 2.06 | |
| Fe2O3 | 0.69% | 0.01 | |
| LOI | 13.11% | n/a | |
| Oxide Weight | 233.70 | ||
| Formula Weight | 268.96 | ||
A general purpose air floated kaolin of good casting properties. It is an appropriate selection for mechanical forming applications where more plasticity is desirable and fired color is not critical.
Bulk Density: 30 lb/cu. ft.
Moisture: 1%
PCE: 34
C.E.C.: 3.5
Specific Gravity: 2.62
pH (10% solids, max.): 6.0
Viscosity (70% solids, cps): 1000
Wet Sieve Residue, +325 mesh (%): 1.0
Median Particle Diameter (microns): 1.2
Specific Surface Area (sq. meters/gram): 17.31
Particle Size (% finer than):
20 microns: 93.6
10: 84.3
5: 73.1
2: 57.8
1: 46.8
0.5: 32.9
| URLs |
http://www.zemex.com/feldspar/master.html
Zemex Feldspar Data Sheets |
| Materials |
Mastercast Kaolin
|
| Materials |
Masterfloat Kaolin
|
| Materials |
Kaolin
The purest of all clays in nature. Kaolins are used in porcelains and stonewares to impart whiteness, in glazes to supply Al2O3 and to suspend slurries. |
| Typecodes |
Kaolin
Pure clay mineral, there are many brand names of varying purity and iron content. |
![]() PayPal | No tracking, No ads, No paywall, No transient content! Just organized, concise information constantly updated and improved. Was this helpful? Consider supporting me. |
| By Tony Hansen Follow me on ![]() | ![]() |
Buy me a coffee and we can talk