Description: Leadless Frit
| Oxide | Analysis | Formula | Tolerance |
|---|---|---|---|
| CaO | 13.97% | 0.67 | |
| K2O | 0.41% | 0.01 | |
| MgO | 0.76% | 0.05 | |
| Na2O | 6.33% | 0.27 | |
| B2O3 | 13.92% | 0.53 | |
| Al2O3 | 9.75% | 0.26 | |
| SiO2 | 54.86% | 2.44 | |
| Oxide Weight | 267.15 | ||
| Formula Weight | 267.15 | ||
| Materials |
Fusion Frit F-19
A commonly available calcium borosilicate frit having a similar chemistry to Ferro Frit 3124. |
| Materials |
Hommel Frit 378A
|
| Materials |
Pemco Frit P-311
|
| Materials |
General Frit GF-113
|
| Materials |
Frit
Frits are made by melting mixes of raw materials, quenching the melt in water, grinding the pebbles into a powder. Frits have chemistries raw materials cannot. |
| Materials |
Ferro Frit 3124
A commonly available calcium borosilicate frit. It is glaze-like, needing only a kaolin addition to create a low-temperature glossy glaze. |
| Typecodes |
Frit
A frit is the powdered form a man-made glass. Frits are premelted, then ground to a glass. They have tightly controlled chemistries, they are available for glazes of all types. |
| Co-efficient of Linear Expansion | 7.7 x 10-6 (50-450C) |
|---|---|
| Co-efficient of Linear Expansion | 7.7 x 10 -6 |
| Frit Softening Point | 1550F |
| Frit Melting Range (C) | 1550F |