| Oxide | Analysis | Formula | Tolerance |
|---|---|---|---|
| K2O | 1.20% | 0.06 | |
| Li2O | 5.90% | 0.90 | |
| Na2O | 0.61% | 0.04 | |
| Al2O3 | 25.40% | 1.13 | |
| SiO2 | 64.40% | 4.86 | |
| Fe2O3 | 2.30% | 0.07 | |
| LOI | 0.20% | n/a | |
| Oxide Weight | 452.52 | ||
| Formula Weight | 453.43 | ||
Was mined at Foote Lithium Co. Mine, Kings Mountain, Cleveland Co., North Carolina, USA from a lithia bearing-pegmatite (quartz-microcline-spodumene pegmatite) since 1938. No longer available.
Sieve Analysis:
+50 mesh: 3.4
+70: 6.3
+100: 10.2
+140: 15.3
+200: 19.0
| Materials |
Spodumene Concentrate
|
| Materials |
Australian Spodumene
|
| Materials |
CGS 3.1 Spodumene
|
| Materials |
SC 1.1 Spodumene
|
| Materials |
SC 1.2 Spodumene
|
| Materials |
UGS Spodumene
|
| Materials |
FSC 2.1 Spodumene
|
| Materials |
Low Melt Spodumene
|
| Materials |
Spodumene
Spodumene is a lithium sourcing feldspar, an alternative to lithium carbonate to supply Li2O to ceramic glazes. Contains up to about 8% Li2O. |
| Typecodes |
Feldspar
The most common source of fluxes for high and medium temperature glazes and bodies. |