K-200 Feldspar

Alternate Names: K200 Feldspar

Description: POTASSIUM/SODIUM/CALCIUM FELDSPAR

Oxide Analysis Formula Tolerance
CaO 0.18% 0.02
K2O 10.13% 0.65
Na2O 3.36% 0.33
Al2O3 17.84% 1.06
SiO2 67.99% 6.86
Fe2O3 0.08% -
LOI 0.31%n/a
Oxide Weight 603.74
Formula Weight 605.61

Notes

K-200 is a high quality feldspar ground to 200 mesh for ceramic applications. It has one of the highest potassium contents of any spar. Carefully beneficiated and controlled for quality, K-200 offers high potash content and low iron oxide per unit of alumina.

Sieve Analysis (Cum):
+200 mesh: 0.3%
+325 mesh: 3.2%

Average Particle Size: 10.1 microns
Specific Surface Area: 1.88 square meters per gram
Bulk Density: 62 lbs/cu ft loose, 74 packed

Related Information

Links

Typecodes Feldspar
The most common source of fluxes for high and medium temperature glazes and bodies.

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://digitalfire.com, All Rights Reserved
Privacy Policy