Description: Cedar Heights Fireclay
| Oxide | Analysis | Formula | Tolerance |
|---|---|---|---|
| CaO | 0.20% | 0.01 | |
| MgO | 0.40% | 0.04 | |
| K2O | 2.10% | 0.08 | |
| Na2O | 0.20% | 0.01 | |
| TiO2 | 1.50% | 0.07 | |
| Al2O3 | 27.30% | 1.00 | |
| SiO2 | 57.80% | 3.59 | |
| Fe2O3 | 1.70% | 0.04 | |
| LOI | 8.80% | n/a | |
| Oxide Weight | 340.75 | ||
| Formula Weight | 373.63 | ||
Medium buff burning fireclay available in 12 and 30 mesh sizes.
| Materials |
Goldart
|
| Materials |
Ceramic Fireclay
|
| Materials |
Bonding Clay
|
| Materials |
CKR Clay
|
| Materials |
Fireclay
|
| Typecodes |
Fireclay
Fireclays are non-kaolin non-ball clay materials similar to stoneware clays but lacking fluxing oxides. Many fireclays have a PCE of 28 or more. |
| Pyrometric Cone Equivalent | 29 |
|---|