1-9 | A | B | C | D | E | F | Frits | G | H | I | J | K | L | M | N | O | P | Q | R | S | T | U | V | W | X | Y | Z

GP K-59 Pottery Plaster

Notes

Georgia-Pacific K-59 Pottery Plaster looks like the closest direct replacement for USG No. 1 Pottery Plaster. The published numbers are strikingly close:

Oxide Analysis Formula Tolerance
Property USG No. 1
Pottery Plaster
GP K-59
Pottery Plaster
Water : plaster 70 : 100 68–70 : 100
Vicat set 14–24 min 25–35 min
Dry density 69 lb/ft³ 69–71 lb/ft³
Dry compressive
strength
2400 psi 2000–2600 psi
Set expansion 0.21% max 0.22–0.27%

USG describes No. 1 as its standard high-strength pottery plaster for slip casting and jiggering. Georgia-Pacific's published K-59 data describes it as intended for all types of potteries and sanitaryware, producing smooth, pinhole-free casts. It can reportedly be mixed as low as 64 parts water where exceptionally strong, long-wearing molds are wanted, although the normal published consistency is 68–70.

The most important number may be the normal consistency. Both products operate around 70 parts water per 100 plaster. That strongly influences the resulting mold's porosity, absorption and strength. This means a potter accustomed to No. 1 should not have to fundamentally rethink mold-making technique when moving to K-59. The dry densities are essentially identical, and the compressive-strength ranges overlap almost perfectly. The expansion of K-59 is slightly higher, but not dramatically so. The obvious difference is set time. K-59's stated 25–35-minute Vicat set is noticeably slower than No. 1's 14–24 minutes. That may actually be convenient for larger molds, but production shops would need to account for it.

Related Information

2026 Great Plaster Squeeze Continues:

A crisis in North American ceramics


Create at Gemini by a submission of the text from this post. AI Policy

This picture has its own page with more detail, click here to see it.

USG specialty plaster is entering a final-inventory phase in the ceramic supply chain, and rationing has begun at some suppliers even though the Southard plant does not close until November.

Nov 19: No meaningful new evidence on GP ability to absorb the industrial-plaster demandUSG's Southard closure has initiated no new announcement from GP confirming increased K-59 production, expanded Blue Rapids manufacturing capacity, additional production shifts, or improved delivery commitments.
Oct 26: At least one online supplier is listing Arcosa pottery plaster on their site for sale.Seattle Pottery Supply plaster listing (their store claims hundreds of bags in stock)
Oct 12: Arcosa appears to be ramping up to produce their equivalent to USG No. 1 . Arcosa Pottery Plaster consistency and strength make it a credible No. 1 replacement. The higher published maximum expansion could matter for dimensionally controlled molds, jigger tooling and multi-part mold registration. The data sheet does not quantify absorption rate, saturation behavior or expected casting turns, so equivalence is not yet established.
Oct 10: Industrial plaster shortages now reported beyond ceramics . A significant new industry report strengthens the evidence that North America's specialty-plaster supply chain is already struggling to absorb the impending closure of USG's Southard operation.
Sept 21: Industrial supplier freemansupply.com posts USG closure notices They state: "With the upcoming closure of U.S. Gypsum (USG), Freeman's plaster and cement supplier, we have been sourcing alternatives to continue supplying the industry with quality products. If you are interested in plaster or cement, please complete this form to be contacted when suitable alternatives are available".
Sept 17: GP requiring full load orders, actively staffing A distributor reports that GP is requiring no mixing of types on orders. GP is recruiting production at the Blue Rapids, Kansas facility specifically for continuous manufacturing of plaster products. 12-hour shifts, including weekends, holidays, and overtime.
Sept 14: Arcosa emerges as another replacement source Brackers Good Earth Clays says it has opened an account with Arcosa Specialty Materials and placed its first truckload order for pottery plaster plus a product comparable to Hydrocal White, due to arrive in October
Sept 9: Various distributors have no K-59 in stock The persistent K-59 shortages at ceramic suppliers suggest that distribution or production is not yet keeping pace with the emerging ceramic-market shift.
Sept 6: USG online store has an “LIMITED INVENTORY” notice It states that availability of USG plasters and gypsum cements is limited and that once a product sells out, it will no longer be available and will be discontinued. Interestingly, significant final inventory remains: 312 bags of No. 1 Pottery Plaster, 218 Hydro-Stone, 123 Ultracal 30 and 95 Hydrocal White, all in 47.5-lb bags. These are being offered for sale while supplies last. The main USG website and CGC pages still have ordinary-looking product listings for No. 1 Pottery Plaster, Cerami-Cal and other products, without conspicuous discontinuation notices.
Sept 2: GP announces close of a plant Georgia-Pacific officially announced that it will permanently close its Tacoma, Washington gypsum plant, affecting 125 employees. GP says weak repair/remodel demand is the reason, and importantly says it expects to continue satisfying customer demand from its remaining facilities. The Tacoma operation is a gypsum-board plant, not the Blue Rapids industrial-plaster operation associated with K-59, so this does not indicate that K-59 production is being cut. But it does show GP is actively rationalizing its gypsum manufacturing network rather than broadly expanding it at this moment.
Sept 1: A distributor is out of USG products It reports that it is completely out of USG No. 1 Pottery Plaster, Hydro-Stone and 20 Minute Casting Plaster, with only a limited amount of Hydrocal White remaining.
Aug 31: GP K-59 sold out at some suppliers Several Canadian suppliers are already showing Georgia-Pacific K-59 as sold out. Another still has 10 of K-59 available, compared with 172 bags of USG No. 1 Pottery Plaster still in stock. That suggests demand may already be shifting toward K-59 faster than some distributors can replenish it.
A signal from Georgia-Pacific itself: Its Blue Rapids, Kansas Industrial Plasters facility, the plant historically associated with K-59, is actively hiring maintenance personnel, including for a rotating 12-hour schedule, with the job posting emphasizing equipment reliability, production optimization and operating performance. Georgia-Pacific’s official industrial-plaster site continues to present pottery plaster as a core business and says it supplies sanitaryware and dinnerware manufacturers and produces both alpha- and beta-gypsum plasters. I still find no announcement of a production increase, additional shifts, capacity expansion, new warehouses, or a specific commitment to replace USG’s Southard volume.
Aug 29: One supplier is imposing anti-hoarding restrictions It will serve normal requirements of existing customers, but will not sell plaster to new customers or permit purchases substantially above usual volumes. It is investigating alternative sources. Another is now limiting Hydro-Stone purchases to 100 lb per customer per week. USG and CGC themselves still have active product pages for No. 1 Pottery Plaster, Hydro-Stone and Ultracal 30, with no visible discontinuation notice, so their public website continues to lag what distributors are reporting.
Aug 19: News from Australia An Australian industrial supplier now states that USG is “phasing out its entire Industrial Products range” made at Southard, that USG has confirmed these products will not be manufactured at another site, and that USG is no longer accepting orders.

Links

URLs https://gpindustrialplasters.com/pottery-plaster/
Georgia-Pacific Industrial Plasters
Materials USG No. 1 Pottery Plaster
Materials Arcosa Pottery Plaster

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://digitalfire.com, All Rights Reserved
Privacy Policy