Description: Leadless high sodium frit for cone 06-02
| Oxide | Analysis | Formula | Tolerance |
|---|---|---|---|
| CaO | 0.30% | 0.02 | |
| K2O | 7.20% | 0.25 | |
| Na2O | 13.00% | 0.69 | |
| ZnO | 1.00% | 0.04 | |
| B2O3 | 16.60% | 0.79 | |
| Al2O3 | 12.60% | 0.41 | |
| SiO2 | 47.70% | 2.61 | |
| F | 1.60% | 0.28 | |
| Oxide Weight | 329.23 | ||
| Formula Weight | 329.23 | ||
| Materials |
Hommel Frit 259
|
| Materials |
Ferro Frit 3269
|
| Materials |
Pemco Frit P-25
|
| Materials |
Fusion Frit FZ-25
|
| Materials |
Frit
Frits are made by melting mixes of raw materials, quenching the melt in water, grinding the pebbles into a powder. Frits have chemistries raw materials cannot. |
| Typecodes |
Frit
A frit is the powdered form a man-made glass. Frits are premelted, then ground to a glass. They have tightly controlled chemistries, they are available for glazes of all types. |
| Co-efficient of Linear Expansion | 10.30 |
|---|---|
| Co-efficient of Linear Expansion | 10.3 x 10-6 |
| Frit Softening Point | 1400F |