Alternate Names: L-17662B
Description: Zinc barium artware and tile glaze frit
| Oxide | Analysis | Formula | Tolerance |
|---|---|---|---|
| BaO | 7.90% | 0.11 | |
| CaO | 8.80% | 0.33 | |
| K2O | 0.60% | 0.01 | |
| Na2O | 4.50% | 0.15 | |
| ZnO | 15.80% | 0.40 | |
| ZrO2 | 10.20% | 0.17 | |
| B2O3 | 10.00% | 0.30 | |
| Al2O3 | 0.90% | 0.02 | |
| SiO2 | 39.50% | 1.37 | |
| F | 1.90% | 0.21 | |
| Oxide Weight | 207.91 | ||
| Formula Weight | 207.91 | ||
| Materials |
Pemco Frit P-64
|
| Materials |
Fusion Frit FZ-30
|
| Materials |
Frit
Frits are made by melting mixes of raw materials, quenching the melt in water, grinding the pebbles into a powder. Frits have chemistries raw materials cannot. |
| Materials |
Hommel Frit G-26
|
| Typecodes |
Frit
A frit is the powdered form a man-made glass. Frits are premelted, then ground to a glass. They have tightly controlled chemistries, they are available for glazes of all types. |
| Co-efficient of Linear Expansion | 8.60 |
|---|---|
| Frit Melting Range (C) | 1500F |