Albion Sperse

Description: Kaolin

Oxide Analysis Formula Tolerance
CaO 0.24% 0.01
K2O 0.60% 0.02
MgO 0.24% 0.02
Na2O 0.56% 0.03
TiO2 0.71% 0.03
Al2O3 35.52% 1.00
SiO2 45.65% 2.18
Fe2O3 1.25% 0.02
LOI 15.22%n/a
Oxide Weight 243.43
Formula Weight 287.13

Notes

Albion Sperse is a coarse-grained, air-floated Georgia kaolin which is highly adaptable to slip-casting and filter press operations. It is unique for its high level of pure kaolinite and coarse particle distribution curve. It features excellent dispersion characteristics, low shrinkage, and a clean white fired color.

Albion Sperse is especially suitable for the manufacture of sanitary ware, oxide color pigments, high tension electric porcelain, and art pottery.

Fired Properties
================
PCE: 34
Fusion Point: 3200F

Cone 5 8 10 12
------------------------------------------------------
Linear Shrinkage (dry basis %): 6.4 8.2 9.3 10.4
*Modulus of Rupture, (psi): 80 30 100 55
Water Absorption, (%): 24.7 20.3 17.9 15.6
Porosity (%): 40.0 35.5 32.8 29.5
Bulk Density (gm/cc): 1.61 1.78 1.83 1.91
Brightness (% reflectance): 90.2 87.0 85.4 82.0
Whiteness (% reflectance): 4.1 6.2 7.4 9.0
Apparent Specific
Gravity (gm/cc): 2.7 2.7 2.73 2.72

*50% clay:50% kaolin

Unfired Properties
==================
Specific Gravity (gm/cc): 2.6
Water of Plasticity (%): 29.1
Modulus of Rupture (psi): 20
Brightness: 78
Whiteness: 26.9
pH (28% solids): 5.1

Particle Size Distribtion:

Minus 20 microns: 97.2
-10: 90.3
-5: 72.9
-2: 48.3
-1: 30.8
-0.5: 17.0
-0.2: 9.5

Mean Particle Size (microns): 2

C.E.C. (meq/100 gm): 20.7

Minimum Dispersed Viscosity, cps:
30% solids Brookfield, No. 2 Spindle, 100 RPM: 16

Relative Settling Rate (in/min Baroid Filter Press): 0.035

Related Information

Links

Materials Kaolin
The purest of all clays in nature. Kaolins are used in porcelains and stonewares to impart whiteness, in glazes to supply Al2O3 and to suspend slurries.
Typecodes Kaolin
Pure clay mineral, there are many brand names of varying purity and iron content.

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://digitalfire.com, All Rights Reserved
Privacy Policy