Pyrax HS

Alternate Names: Pyrax HS#5

Description: Pyrophyllite

Oxide Analysis Formula Tolerance
K2O 2.30% 0.18
Na2O 0.40% 0.05
TiO2 0.10% 0.01
Al2O3 13.80% 1.00
SiO2 80.90% 9.95
Fe2O3 0.20% 0.01
LOI 2.30%n/a
Oxide Weight 722.13
Formula Weight 739.13

Notes

Described by the manufacturer as a high sericite pyrophyllite for sanitaryware which aids in early mullite formation offering increased fired strength, faster firing cycles, and increased thermal shock resistance.

Pyrax MP, another grade, is used in rapid fire ceramic wall tile bodies. It lowers firing temperature, produces low moisture expansion bodies with good craze resistance, increases thermal shock resistance, and greatly increases firing strength in vitreous bodies.

Related Information

Links

Materials Pyrophyllite
A refractory aluminum silicate mineral often used in clay body recipes to lower thermal expansion, control fired maturity, mullite development catalyst, etc.
Materials Pyrax Pyrophyllite
Materials Pyrax RG
Typecodes Aluminum Silicate
Materials not classifiable as commonly known aluminum silicates. For example, kaolin is a common aluminum silicate.
URLs https://www.vanderbiltminerals.com/resources/Minerals_and_Chemical_for_Ceramics_and_Refractories_web.pdf
Vanderbilt Minerals for Ceramics Technical Sheet
Includes Vansil, Pyrax, Peerless, Dixie, Veegum, Vanzan, Darvan.

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://digitalfire.com, All Rights Reserved
Privacy Policy