Prestige AK

Alternate Names: Prestige Ball Clay

Description: Ball clay

Oxide Analysis Formula Tolerance
SiO2 51.50% 2.77
Al2O3 31.50% 1.00
TiO2 1.00% 0.04
Fe2O3 1.10% 0.02
CaO 0.10% 0.01
MgO 0.30% 0.02
K2O 1.90% 0.07
Na2O 0.30% 0.02
LOI 1.90%n/a
Oxide Weight 283.98
Formula Weight 322.71

Notes

A composite blend clay specially formulated for porous earthenware. Suitable also for many engobe recipes.

Related Information

Links

Minerals Kaolinite
The most fundamental clay mineral. This mineral is found in nature in its purest form as kaolin. How
Minerals Quartz
Quartz is the most abundant mineral on earth, it is the main crystalline mineral form of silica (SiO
Minerals Potash Mica
Minerals Soda Mica
Typecodes Ball Clay
Ball clays are abundant and very plastic and are used in all types of plastic forming bodies. They are not as white-burning or refractory as kaolins but lower in iron and fluxes than bentonites.

Data

Sieve Analysis Wet 0.3% residue on 125 µm screen
Co-efficient of Linear Expansion 49 x 10-7 (25C-500C prefired at 1200C)
Ultimate Particle Size Distribution 1 micron: 73% underside 2 microns: 81% 5 microns: 92% 10 microns: 95% 20 microns: 98%
Modulus of Rupture - Fired 63.2 kgf/cm2

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://digitalfire.com, All Rights Reserved
Privacy Policy