Description: Noodled refined Devon ball clay
| Oxide | Analysis | Formula | Tolerance |
|---|---|---|---|
| CaO | 0.20% | 0.01 | |
| K2O | 2.20% | 0.10 | |
| MgO | 0.30% | 0.03 | |
| Na2O | 0.30% | 0.02 | |
| TiO2 | 1.50% | 0.08 | |
| Al2O3 | 24.30% | 1.00 | |
| SiO2 | 63.10% | 4.41 | |
| Fe2O3 | 0.90% | 0.02 | |
| LOI | 7.20% | n/a | |
| C | 0.60% | n/a | |
| Oxide Weight | 389.53 | ||
| Formula Weight | 422.48 | ||
Particle Size (e.s.d.)
125 microns - 0.05
10 microns - 92
2 microns - 68
1 microns - 58
Modulus of Rupture at 110C
Mn/M2 - 6.6
lbf/in2 - 950
Defloculant Required - (3:1 Na2SiO3(C.100):Na2CO3) - 0.1
Water Absorption
1120C - 4.0
1220C - 0.00
Shrinkage Dry to Fired
1120C - 10.00
1220C - 12.50
Reflectance 464nm
1120C - 70
1220C - 45
Refractoriness
Cone - 30, 1670C
| Materials |
Ball Clay
A fine particled highly plastic secondary clay used mainly to impart plasticity to clay and porcelain bodies and to suspend glaze, slips and engobe slurries. |
| Typecodes |
Ball Clay
Ball clays are abundant and very plastic and are used in all types of plastic forming bodies. They are not as white-burning or refractory as kaolins but lower in iron and fluxes than bentonites. |
![]() PayPal | No tracking, No ads, No paywall, No transient content! Just organized, concise information constantly updated and improved. Was this helpful? Consider supporting me. |
| By Tony Hansen Follow me on ![]() | ![]() |
Buy me a coffee and we can talk