Description: Tennessee Ball Clay

Oxide Analysis Formula Tolerance
CaO 0.30% 0.02
K2O 1.20% 0.05
MgO 0.30% 0.03
Na2O 0.20% 0.01
TiO2 1.50% 0.07
Al2O3 28.10% 1.00
SiO2 57.40% 3.47
Fe2O3 0.80% 0.02
LOI 10.20%n/a
Oxide Weight 325.96
Formula Weight 362.99

Notes

This is sold by Chemical Distributors Inc. to be used in a 50:50 mix with Texas Pioneer Talc.
It is a mixture of 75% SGP Ball Clay and 25% OM#4 Ball Clay.

Related Information

Links

Materials Ball Clay
A fine particled highly plastic secondary clay used mainly to impart plasticity to clay and porcelain bodies and to suspend glaze, slips and engobe slurries.
Typecodes Ball Clay
Ball clays are abundant and very plastic and are used in all types of plastic forming bodies. They are not as white-burning or refractory as kaolins but lower in iron and fluxes than bentonites.

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://digitalfire.com, All Rights Reserved
Privacy Policy