1-9 | A | B | C | D | E | F | Frits | G | H | I | J | K | L | M | N | O | P | Q | R | S | T | U | V | W | X | Y | Z

F7/SE Feldspar

Alternate Names: Feldspar Soda F7/SE

Description: Soda Feldspar

Oxide Analysis Formula Tolerance
CaO 0.55% 0.05
MgO 0.05% 0.01
K2O 0.28% 0.02
Na2O 10.20% 0.92
TiO2 0.06% -
Al2O3 17.50% 0.96
SiO2 70.80% 6.60
Fe2O3 0.12% -
LOI 0.36%n/a
Oxide Weight 557.66
Formula Weight 559.67

Related Information

Links

Minerals Quartz
Quartz is the most abundant mineral on earth, it is the main crystalline mineral form of silica (SiO
Minerals Na-Feldspar
Most common feldspars contain both sodium and potassium. The term Na-Feldspar designates one where t
Materials Soda Feldspar
A feldspar having a KNaO content that predominates in sodium.
Typecodes Feldspar
The most common source of fluxes for high and medium temperature glazes and bodies.

Data

Bulk Density g/cc (Packed) 1.2
Hardness (Moh) 6.5
Ultimate Particle Size Distribution >71 micron: 1%
Density (Specific Gravity) 2.65
pH for dry powder 8-9

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://digitalfire.com, All Rights Reserved
Privacy Policy