Sil-o-spar

Description: Potash/sodium/calcium Feldspar

Oxide Analysis Formula Tolerance
CaO 1.05% 0.15
K2O 2.86% 0.24
Na2O 4.86% 0.61
Al2O3 13.47% 1.04
SiO2 77.37% 10.10
Fe2O3 0.06% -
LOI 0.07%n/a
Oxide Weight 781.94
Formula Weight 782.49

Notes

Sil-O-Spar is a high quality blend of sodium/potassium/calcium aluminum silicate (feldspar) and silica, ground to 170 mesh, for ceramic applications. Carefully beneficiated and controlled for quality, Sil-O-Spar provides the advantages of pre-blended and uniformly sized non-plastic flux with low iron oxide content. Its coarse particle size makes it an ideal choice for casting slips.

Related Information

Links

URLs http://www.zemex.com/feldspar/silospar.html
Silospar Data Sheet
Materials F-20 Feldspar
Materials G-20 Feldspar
Materials G-200 Feldspar
Materials NC-4 Feldspar
Materials Calcium Feldspar
Materials Potash Feldspar
A feldspar having a KNaO content that predominates in potassium.
Materials Soda Feldspar
A feldspar having a KNaO content that predominates in sodium.
Typecodes Feldspar
The most common source of fluxes for high and medium temperature glazes and bodies.

Data

Apparent Viscosity (cps) 14.37
Bulk Density lbs/cu. ft. (Packed) 37 loose, 87 packed
Sieve Analysis Dry +200 mesh: 2.78% +325 mesh: 11.43%
Surface Area (m2/gm) 1.13
pH for dry powder 9