Description: SANITARY WARE SLURRY
| Oxide | Analysis | Formula | Tolerance |
|---|---|---|---|
| CaO | 0.10% | 0.01 | |
| K2O | 1.40% | 0.06 | |
| MgO | 0.30% | 0.03 | |
| Na2O | 0.16% | 0.01 | |
| TiO2 | 1.61% | 0.09 | |
| Al2O3 | 24.05% | 1.00 | |
| SiO2 | 60.87% | 4.30 | |
| Fe2O3 | 1.01% | 0.03 | |
| LOI | 10.28% | n/a | |
| Oxide Weight | 379.58 | ||
| Formula Weight | 423.08 | ||
This slurry is intended to enhance casting qualities with faster casting rate as well as faster dewatering and set-up.
Crude Color: Dark Brown
% Solids: 60-61
Dry M.O.R. (psi 50% clay/50% flint, cast bars): 520
Water of Plasticity (%): 33
Linear Dry Shrinkage (%): 5.6
Soluble Sulfates (ppm): 800-1200
Filtration (ml): 34
Specific Surface Area (sq meters per gram): 15.8
CEC/MBI (meq/100 ml): 7.0-7.5
pH @90F: 4.5-5.8
Specific Gravity: 1.59-1.61
Viscosity @ 90F (cps Brookfield, 100 rpm, spindle 3): 450-750
Casting Rate @ 90F, 15 min. (g): 45
Deflocculant Type: Sodium Silicate "N" Brand
Particle Size (% finer than):
5 microns: 77
1 micron: 44
0.5 microns: 33
| Typecodes |
Ball Clay
Ball clays are abundant and very plastic and are used in all types of plastic forming bodies. They are not as white-burning or refractory as kaolins but lower in iron and fluxes than bentonites. |