Solargil Frit FR8

Description: Calcium borate frit

Oxide Analysis Formula Tolerance
CaO 17.97% 0.68
K2O 4.88% 0.11
Na2O 6.13% 0.21
B2O3 20.01% 0.61
Al2O3 1.45% 0.03
SiO2 49.56% 1.75
Oxide Weight 212.32
Formula Weight 212.32

Related Information

Links

Materials Frit
Frits are made by melting mixes of raw materials, quenching the melt in water, grinding the pebbles into a powder. Frits have chemistries raw materials cannot.
Materials Ferro Frit 3134
A frit with 23% B2O3. The most common of frits used in pottery in North America. Around the world, other companies make frits of equivalent chemistry.
Materials Fusion Frit F-12
Typecodes Frit
A frit is the powdered form a man-made glass. Frits are premelted, then ground to a glass. They have tightly controlled chemistries, they are available for glazes of all types.

Data

Co-efficient of Linear Expansion 84.9 x 10-7 C (Appen)
Frit Softening Point 920-1000C

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://digitalfire.com, All Rights Reserved
Privacy Policy