Alternate Names: PotteryCrafts Frit 3110
Description: This is actually Ferro Frit 3110
| Oxide | Analysis | Formula | Tolerance |
|---|---|---|---|
| CaO | 6.30% | 0.29 | |
| K2O | 2.30% | 0.06 | |
| Na2O | 15.30% | 0.64 | |
| B2O3 | 2.60% | 0.10 | |
| Al2O3 | 3.70% | 0.09 | |
| SiO2 | 69.80% | 3.03 | |
| Oxide Weight | 260.76 | ||
| Formula Weight | 260.76 | ||
| Materials |
Frit
Frits are made by melting mixes of raw materials, quenching the melt in water, grinding the pebbles into a powder. Frits have chemistries raw materials cannot. |
| Materials |
Ferro Frit 3110
High sodium, high thermal expansion low boron frit. A super-feldspar in clay bodies. Melts at very low temperatures. Useful to make crackle glazes. |
| Typecodes |
Frit
A frit is the powdered form a man-made glass. Frits are premelted, then ground to a glass. They have tightly controlled chemistries, they are available for glazes of all types. |
| Co-efficient of Linear Expansion | 10.1 |
|---|---|
| Frit Melting Range (C) | 920-950C |
![]() PayPal | No tracking, No ads, No paywall, No transient content! Just organized, concise information constantly updated and improved. Was this helpful? Consider supporting me. |
| By Tony Hansen Follow me on ![]() | ![]() |
Buy me a coffee and we can talk