Oxide Analysis Formula Tolerance
CaO 0.04% -
K2O 1.60% 0.05
MgO 0.22% 0.01
Na2O 0.06% -
TiO2 0.30% 0.01
Al2O3 37.50% 1.00
SiO2 47.50% 2.15
Fe2O3 0.65% 0.01
LOI 12.30%n/a
Oxide Weight 239.01
Formula Weight 272.53

Notes

Particle Size Distribution:
>53 microns: 0.1 max
>10 microns: 8
<2 microns: 61

Modulus of Rupture, Kgf/cm2:
At 80% Relative Humidity: 10.0
Dried at 110C: 21.0

Casting Rate @ 65% solids (mm2/min): 0.35
% P84 Deflocculant Required for 5 Poise Slip: 0.4

1180C 1280C
Fired Absorption: 20% 11%
Fired Shrinkage: 7% 11.5%
Brightness: 90 88

Related Information

Links

Typecodes Kaolin
Pure clay mineral, there are many brand names of varying purity and iron content.

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://digitalfire.com, All Rights Reserved
Privacy Policy