Alternate Names: NA200, MC NA 200
| Oxide | Analysis | Formula | Tolerance |
|---|---|---|---|
| SiO2 | 64.84% | 5.55 | |
| Al2O3 | 20.71% | 1.04 | |
| Fe2O3 | 0.06% | - | |
| CaO | 1.82% | 0.17 | |
| Na2O | 6.49% | 0.54 | |
| K2O | 5.20% | 0.28 | |
| BaO | 0.33% | 0.01 | |
| LOI | 0.40% | n/a | |
| Oxide Weight | 511.38 | ||
| Formula Weight | 513.43 | ||
The company was introducing this January 2007 and claimed: "A high quality sodium/potassium/calcium aluminum silicate, ground to 200 mesh for ceramic applications. Carefully beneficiated and controlled for quality, it offers a high alkali content and low iron oxide content per unit of alumina."
Cone 11 fired flow tests beside MC K-325 show this to melt much better even though it is a larger particle size. It also melts much better than Custer or G-200 and the melt flow is whiter than G-200 and much whiter than Custer.

This picture has its own page with more detail, click here to see it.
Our melt fluidity tester is being used to compare cone 8 melt fluidities of Custer, G-200 and i-Minerals high soda and high potassium feldspars. Notice how little the pure materials are moving (bottom), even though they are fired to cone 11. In addition, the sodium feldspars move better than the potassium ones. But feldspars do their real fluxing work when they can interact with other materials. As a demonstration of that, note how well they flow with only 10% frit added (top), even though fired three cones lower.
| Materials |
Potash Feldspar
A feldspar having a KNaO content that predominates in potassium. |
| Materials |
Soda Feldspar
A feldspar having a KNaO content that predominates in sodium. |
| Typecodes |
Feldspar
The most common source of fluxes for high and medium temperature glazes and bodies. |
| Bulk Density lbs/cu. ft. (Packed) | 90 |
|---|---|
| Sieve Analysis Dry | +140 mesh: 0.5 max +200: 1.5 max +325: 10.0 max |