Oct 22, 2026: We are working on protecting our servers against the PHP2Shell vulnerability just discovered. The CDN download server is back online. The digitalfire and insight-live servers were patched on Oct 21.

1-9 | A | B | C | D | E | F | Frits | G | H | I | J | K | L | M | N | O | P | Q | R | S | T | U | V | W | X | Y | Z

Kentucky 4&12 Ball

Description: Kentucky Ball Clay

Oxide Analysis Formula Tolerance
CaO 0.30% 0.02
K2O 0.90% 0.04
MgO 0.50% 0.05
Na2O 0.20% 0.01
TiO2 1.50% 0.07
Al2O3 27.00% 1.00
SiO2 55.40% 3.48
Fe2O3 1.00% 0.02
LOI 13.20%n/a
Oxide Weight 327.91
Formula Weight 377.78

Notes

A fine-grained ball clay known for its excellent strength and plasticity in casting bodies. Kentucky 4 & 12 is used primarily used in the sanitaryware industry..

Physical Properties
===================
Water of Plasticity*: 37.0%
% Dry Shrinkage*: 6.5
Dry M.O.R., psi:* 825
pH: 4.4
C.E.C., meq/100g: 11.0
Specific Surface Area, sq metre/g: 24.4
Soluble sulfur+: Low

P.C.E.: 32

Particle Size, Microns: 20 10 5 2 1 0.5 0.2
(% finer than) 99% 97% 93% 81% 72% 56% 35%

Fired Properties
================
Cone 5 10
----
Total Shrinkage: 13.0% 14.5%
Absorption: 10.0% 1.0%

------------------
*Extruded, 50% ball clay, 50% flint
+Low-trace to 150, Med-150-400, High-450+
**50% Clay, 50% Nepheline Syenite

Related Information

Links

Typecodes Ball Clay
Ball clays are abundant and very plastic and are used in all types of plastic forming bodies. They are not as white-burning or refractory as kaolins but lower in iron and fluxes than bentonites.

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://digitalfire.com, All Rights Reserved
Privacy Policy