Description: Reimbold & Strick stoneware tableware frit < 1050C
| Oxide | Analysis | Formula | Tolerance |
|---|---|---|---|
| Na2O | 3.00% | 0.14 | |
| SiO2 | 43.00% | 2.08 | |
| SrO | 13.00% | 0.36 | |
| K2O | 2.00% | 0.06 | |
| BaO | 4.00% | 0.08 | |
| B2O3 | 25.00% | 1.04 | |
| ZnO | 10.00% | 0.36 | |
| Oxide Weight | 290.66 | ||
| Formula Weight | 290.66 | ||
| Materials |
Frit
Frits are made by melting mixes of raw materials, quenching the melt in water, grinding the pebbles into a powder. Frits have chemistries raw materials cannot. |
| Typecodes |
Frit
A frit is the powdered form a man-made glass. Frits are premelted, then ground to a glass. They have tightly controlled chemistries, they are available for glazes of all types. |
| Co-efficient of Linear Expansion | 54 x 10-7 (20-400C) |
|---|---|
| Frit Softening Point | 660C |
| Glass Transition Temperature | 600C |