Alternate Names: DakotaPure Mica
Description: muscovite mica
| Oxide | Analysis | Formula | Tolerance |
|---|---|---|---|
| FeO | 1.20% | 0.09 | |
| P2O5 | 0.20% | 0.01 | |
| MgO | 1.30% | 0.21 | |
| CaO | 0.70% | 0.08 | |
| K2O | 6.60% | 0.45 | |
| Na2O | 2.50% | 0.26 | |
| Fe2O3 | 3.10% | 0.12 | |
| Al2O3 | 27.10% | 1.70 | |
| SiO2 | 46.80% | 4.97 | |
| LOI | 5.00% | n/a | |
| SO3 | 0.02% | n/a | |
| Oxide Weight | 571.77 | ||
| Formula Weight | 601.99 | ||
No longer produced since Pacer Corporation ceased operations.
Wasvailable in various sizes. Potters and producers added it to terra cotta clay bodies to create sparkles. Standard grades were much too fine for this effect; the drilling mud grades were better (intended for the flakes to heal leaks the way platelets do in the blood stream). These were called LCM Drilling Mud Mica.
The analysis provided here does not add up to 100, and the manufacturer did not provide an LOI. The highest LOI we could find on a typical mica is 5%, so this was used here. Either the other numbers needed to be scaled up to total 95 or the LOI set to 10.0 to account for unspecified volatile materials.

This picture has its own page with more detail, click here to see it.
An example of how a small addition of mica affects the fired appearance of a terra cotta clay. The effect is still working at cone 03 (left) but is more commonly employed at cone 06 (right). Notice that it is still visible even under the glaze. This body is popular on the west coast, it was designed by D'Arcy Margesson. Standard grades of mica are too fine for the effect, this is likely Custer LCM Drilling Mud Mica.
| URLs |
http://www.pacerminerals.com/dptech.html
Pacer website |
| URLs |
http://mineral.galleries.com/minerals/silicate/micas.htm
The Mica Group of Minerals |
| URLs |
http://en.wikipedia.org/wiki/Mica
Mica at Wikipedia |
| URLs |
http://www.pacerminerals.com/products/oil-well-lcm-mica
Custer Drilling Mud Mica |
| Materials |
Mica
|
| Typecodes |
Aluminum Silicate
Materials not classifiable as commonly known aluminum silicates. For example, kaolin is a common aluminum silicate. |
| Bulk Density lbs/cu. ft. (Packed) | 33.2-A200, 30.9 A-140 |
|---|---|
| Bulk Density lbs/cu. ft. (Packed) | 33.2 |
| Hardness (Moh) | 2.5 |
| Sieve Analysis Dry | A200 Grade: +100: 0.3 +200: 20.4 +325: 35.3 A140 Grade: on 80#: 1.0% on 200#: 58.0% |
| Sieve Analysis Dry | +100: 0.3 +200: 20.4 +325: 35.3 |
| Density (Specific Gravity) | 2.66 |
| pH for dry powder | 8.0 |