Oxide Analysis Formula Tolerance
CaO 0.55% 0.04
MgO 0.70% 0.07
K2O 2.69% 0.11
Na2O 0.63% 0.04
TiO2 1.21% 0.06
Al2O3 27.11% 1.00
SiO2 57.34% 3.59
Fe2O3 1.16% 0.03
SO4 0.12%n/a
LOI 8.19%n/a
Oxide Weight 343.85
Formula Weight 375.01

Related Information

Links

Minerals Kaolinite
The most fundamental clay mineral. This mineral is found in nature in its purest form as kaolin. How
Minerals Quartz
Quartz is the most abundant mineral on earth, it is the main crystalline mineral form of silica (SiO
Materials Clay 215
Materials Clay 220
Materials Clay 216
Materials Clay 222
Materials Clay 232
Materials Clay 233
Materials Clay 244
Materials Clay 220

Data

Dry Strength (kgf/cm2) 25.23
Firing Shrinkage 1150C: 6.13% 1200C: 7.34% 1250C: 7.34% 1325C: 8.14%
Sieve Analysis Dry > 41 micron: 0% > 30 micron: 0.45% > 20 micron: 2.79% > 10 micron: 20.3% < 3 micron: 37.55%

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://digitalfire.com, All Rights Reserved
Privacy Policy