Kaolin Slurry

Oxide Analysis Formula Tolerance
CaO 0.10% -
K2O 0.20% 0.01
MgO 0.05% -
Na2O 0.12% 0.01
TiO2 1.56% 0.05
Al2O3 38.40% 1.00
SiO2 45.30% 2.00
Fe2O3 0.50% 0.01
LOI 13.50%n/a
Oxide Weight 229.05
Formula Weight 264.80

Notes

A carefully controlled kaolin-water suspension formulated for use in ceramic castings.

Physical Properties
===================
Dry M.O.R., psi:* 400
pH: 4.8
C.E.C., meq/100g: 6.5 +/- 1.0
Specific Surface Area, sq metre/g: 16.5
Specific Gravity: 2.6
P.C.E.: 33-34

Particle Size, Microns: 20 10 5 2 1 0.5 325# residue
(% finer than) 99% 97% 93% 81% 72% 56% .5

Fired Properties
================
Color, Cone 8 (L) 83.0
(a) -0.8
(b) 8.6

------------------
*Extruded, 50% ball clay, 50% flint
**50% Clay, 50% Nepheline Syenite

Related Information

Links

Materials Kaolin
The purest of all clays in nature. Kaolins are used in porcelains and stonewares to impart whiteness, in glazes to supply Al2O3 and to suspend slurries.
Typecodes Kaolin
Pure clay mineral, there are many brand names of varying purity and iron content.

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://digitalfire.com, All Rights Reserved
Privacy Policy