1-9 | A | B | C | D | E | F | Frits | G | H | I | J | K | L | M | N | O | P | Q | R | S | T | U | V | W | X | Y | Z

Ferro Frit CC-263

Alternate Names: Frit CC263, Frit CC268, Frit CC-268

Description: Low expansion high CaO balanced boron source

Oxide Analysis Formula Tolerance
CaO 9.00% 0.56
K2O 3.00% 0.11
MgO 1.00% 0.09
Na2O 2.50% 0.14
SrO 3.00% 0.10
ZrO2 0.50% 0.01
B2O3 20.00% 1.00
Al2O3 11.00% 0.38
SiO2 50.00% 2.91
Oxide Weight 349.20
Formula Weight 349.20

Notes

This is a USA pottery frit, Ferro now calls it Frit CC263-2. It is available in small quantities at lagunaclay.com. They call it an "alkaline, alkaline earth alumina borosilicate" and say it is "a well-balanced composition without barium. Typically used as an all-fritted glossy glaze in the general range Orton cone 04-4." This is likely a major constituent in their low fire glazes.

Was formerly #CC268.

Ferro only publishes an approximate analysis as of 2008, however this one was historical (from previous sources).

It is balanced cone 02-1 clear glaze.

Related Information

Links

Materials Frit
Frits are made by melting mixes of raw materials, quenching the melt in water, grinding the pebbles into a powder. Frits have chemistries raw materials cannot.
Materials Ferro Frit CC-263-2
Typecodes Frit
A frit is the powdered form a man-made glass. Frits are premelted, then ground to a glass. They have tightly controlled chemistries, they are available for glazes of all types.
Typecodes Available from Laguna Clays
URLs https://digitalfire.com/4sight/datasheets/ferropotteryfrits2008.pdf
Ferro Pottery Frits 2008

Data

Co-efficient of Linear Expansion 6.79
Frit Softening Point 1650-1850F

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://digitalfire.com, All Rights Reserved
Privacy Policy