Ferro Frit 3292

Alternate Names: F3292

Description: Strontium frit all or partially fritted clear glazes

Oxide Analysis Formula Tolerance
CaO 10.53% 0.54
K2O 3.14% 0.10
Li2O 0.42% 0.04
MgO 0.70% 0.05
Na2O 3.01% 0.14
SrO 4.83% 0.13
B2O3 5.75% 0.24
Al2O3 10.76% 0.30
SiO2 60.86% 2.91
Oxide Weight 287.63
Formula Weight 287.63

Notes

This is a USA pottery frit, Ferro now calls it Frit 3292-2.

Useful addition to first fire sanitary ware. Balanced, can make up the bulk of a recipe.

Related Information

Links

Materials Fusion Frit F-134
Materials Frit
Frits are made by melting mixes of raw materials, quenching the melt in water, grinding the pebbles into a powder. Frits have chemistries raw materials cannot.
Materials Hommel Frit 389
Typecodes Frit
A frit is the powdered form a man-made glass. Frits are premelted, then ground to a glass. They have tightly controlled chemistries, they are available for glazes of all types.
URLs https://digitalfire.com/4sight/datasheets/ferropotteryfrits2008.pdf
Ferro Pottery Frits 2008

Data

Co-efficient of Linear Expansion 7.62
Frit Softening Point 1650-1900F

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://digitalfire.com, All Rights Reserved
Privacy Policy