Alternate Names: Frit KGF4131
Description: A medium to hard unleaded frit
| Oxide | Analysis | Formula | Tolerance |
|---|---|---|---|
| CaO | 11.60% | 0.68 | |
| Na2O | 5.90% | 0.32 | |
| B2O3 | 14.30% | 0.68 | |
| Al2O3 | 10.70% | 0.35 | |
| SiO2 | 57.50% | 3.17 | |
| Oxide Weight | 331.20 | ||
| Formula Weight | 331.20 | ||
A medium to hard unleaded frit suitable for use alone or with others to produce clear glazes. A glaze made of frit and 10% kaolin will have a firing range of 1050 to 1100 deg.C. Adding 10% KGF4064 to this glaze will lower its firing temperature; just as adding a similar amount of silica and/or calcined alumina will increase the firing temperature of the glaze. Also available in milled form (1019663 - KMP4131), milled to a nominal 98% less than 75 microns.

This picture has its own page with more detail, click here to see it.
Some frit companies publish the chemistry of their frits, others do not. Some publish some of their products. Some published in the past but do not do so now. When frit data sheets do not provide an oxide analysis they become an impediment to use in glaze chemistry.
| Materials |
Frit
Frits are made by melting mixes of raw materials, quenching the melt in water, grinding the pebbles into a powder. Frits have chemistries raw materials cannot. |
| Typecodes |
Frit
A frit is the powdered form a man-made glass. Frits are premelted, then ground to a glass. They have tightly controlled chemistries, they are available for glazes of all types. |
| Co-efficient of Linear Expansion | 61 x 10-7 20-500C |
|---|---|
| Frit Softening Point | 670C |
| Glass Transition Temperature | 608C |