Oct 22, 2026: We are working on protecting our servers against the PHP2Shell vulnerability recently discovered. Servers were upgraded ahead of schedule on Oct 21. This could cause some issues. Please contact us if you encounter any.

1-9 | A | B | C | D | E | F | Frits | G | H | I | J | K | L | M | N | O | P | Q | R | S | T | U | V | W | X | Y | Z

Kaolin 151

Alternate Names: Kaolen 151

Oxide Analysis Formula Tolerance
CaO 0.26% 0.01
MgO 0.17% 0.01
K2O 0.13% -
Na2O 0.06% -
TiO2 0.22% 0.01
Al2O3 35.75% 1.00
SiO2 45.31% 2.15
Fe2O3 0.75% 0.01
LOI 16.42%n/a
SO4 0.34%n/a
Oxide Weight 235.81
Formula Weight 283.29

Notes

Available in minus 20cm, -100 microns, -75 microns.

Related Information

Links

Materials Kaolin 115
Materials Kaolin 171
Materials Kaolin 111
Materials Kaolin 113
Materials Kaolin 114
Materials Kaolin 143
Materials Kaolin
The purest of all clays in nature. Kaolins are used in porcelains and stonewares to impart whiteness, in glazes to supply Al2O3 and to suspend slurries.
Typecodes Kaolin
Pure clay mineral, there are many brand names of varying purity and iron content.

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://digitalfire.com, All Rights Reserved
Privacy Policy