CusterMica

Alternate Names: DakotaPure Mica

Description: muscovite mica

Oxide Analysis Formula Tolerance
FeO 1.20% 0.09
P2O5 0.20% 0.01
MgO 1.30% 0.21
CaO 0.70% 0.08
K2O 6.60% 0.45
Na2O 2.50% 0.26
Fe2O3 3.10% 0.12
Al2O3 27.10% 1.70
SiO2 46.80% 4.97
LOI 5.00%n/a
SO3 0.02%n/a
Oxide Weight 571.77
Formula Weight 601.99

Notes

Available in various sizes. It is added to terra cotta clay bodies to create sparkles. Standard grades are much too fine for this effect, use the drilling mud grades (the flakes heal leaks the way platelets do in the blood stream). These are called LCM Drilling Mud Mica.

The analysis provided here does not add up to 100 and the manufacturer does not provide an LOI. The highest LOI we can find on a typical mica is 5%, so this was used. Either the other numbers need to be scaled up to total 95 or the LOI set to 10.0 to account for unspecified volatile materials.

Related Information

Sparkles on clay. Is that possible?


This picture has its own page with more detail, click here to see it.

An example of how a small addition of mica affects the fired appearance of a terra cotta clay. The effect is still working at cone 03 (left) but is more commonly employed at cone 06 (right). Notice that it is still visible even under the glaze. This body is popular on the west coast, it was designed by D'Arcy Margesson. Standard grades of mica are too fine for the effect, this is likely Custer LCM Drilling Mud Mica.

Links

URLs http://www.pacerminerals.com/dptech.html
Pacer website
URLs http://mineral.galleries.com/minerals/silicate/micas.htm
The Mica Group of Minerals
URLs http://en.wikipedia.org/wiki/Mica
Mica at Wikipedia
URLs http://www.pacerminerals.com/products/oil-well-lcm-mica
Custer Drilling Mud Mica
Materials Mica
Typecodes Aluminum Silicate
Materials not classifiable as commonly known aluminum silicates. For example, kaolin is a common aluminum silicate.

Data

Bulk Density lbs/cu. ft. (Packed) 33.2-A200, 30.9 A-140
Bulk Density lbs/cu. ft. (Packed) 33.2
Hardness (Moh) 2.5
Sieve Analysis Dry A200 Grade: +100: 0.3 +200: 20.4 +325: 35.3 A140 Grade: on 80#: 1.0% on 200#: 58.0%
Sieve Analysis Dry +100: 0.3 +200: 20.4 +325: 35.3
Density (Specific Gravity) 2.66
pH for dry powder 8.0

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://digitalfire.com, All Rights Reserved
Privacy Policy