| Oxide | Analysis | Formula | Tolerance |
|---|---|---|---|
| CaO | 0.10% | 0.01 | |
| K2O | 2.40% | 0.09 | |
| MgO | 0.40% | 0.04 | |
| Na2O | 0.30% | 0.02 | |
| TiO2 | 1.30% | 0.06 | |
| Al2O3 | 28.60% | 1.00 | |
| SiO2 | 56.00% | 3.32 | |
| Fe2O3 | 1.00% | 0.02 | |
| LOI | 10.00% | n/a | |
| C | 1.80% | n/a | |
| Oxide Weight | 321.34 | ||
| Formula Weight | 364.33 | ||
Particle Size (e.s.d.)
125 microns - 0.50
10 microns - 97
2 microns - 83
1 microns - 74
Modulus of Rupture at 110C
Mn/M2 - 6.9
lbf/in2 - 1000
Defloculant Required - (3:1 Na2SiO3(C.100):Na2CO3) - 0.3
Water Absorption
1120C - 0.5
1220C - 0.50
Shrinkage Dry to Fired
1120C - 14.00
1220C - 15.00
Reflectance 464nm
1120C - 65
1220C - 40
Refractoriness
Cone - 33, 1730C
| Materials |
Ball Clay
A fine particled highly plastic secondary clay used mainly to impart plasticity to clay and porcelain bodies and to suspend glaze, slips and engobe slurries. |
| Typecodes |
Ball Clay
Ball clays are abundant and very plastic and are used in all types of plastic forming bodies. They are not as white-burning or refractory as kaolins but lower in iron and fluxes than bentonites. |
![]() PayPal | No tracking, No ads, No paywall, No transient content! Just organized, concise information constantly updated and improved. Was this helpful? Consider supporting me. |
| By Tony Hansen Follow me on ![]() | ![]() |
Buy me a coffee and we can talk