WC-5 Kaolin

Oxide Analysis Formula Tolerance
CaO 0.06% -
K2O 0.18% 0.01
MgO 0.05% -
Na2O 0.03% -
TiO2 1.50% 0.05
Al2O3 38.40% 1.00
SiO2 45.60% 2.02
Fe2O3 0.40% 0.01
LOI 13.80%n/a
Oxide Weight 229.02
Formula Weight 265.69

Notes

Wilklay WC-5 is a clean, high quality, very white firing airfloated kaolin especially selected for the whitewares segment of the ceramic industries. The clay has very low residue, an intermediately fine particle size and high plasticity. It is an alternative to #6 Tile and Sapphire kaolin.

Moisture, Max% as produced: 1.0
325 mesh residue, Max: 1.0
Median particle size: 1.2 microns
pH (28% solids), average: 6.9
CEC (Meq/100 gr): 4.0

Particle size:
% Finer than 20 microns: 98
10 microns: 93
5 microns: 80
2 microns: 58
1 micron: 44
0.5 microns: 27

Related Information

Links

Materials Kaolin
The purest of all clays in nature. Kaolins are used in porcelains and stonewares to impart whiteness, in glazes to supply Al2O3 and to suspend slurries.
Typecodes Kaolin
Pure clay mineral, there are many brand names of varying purity and iron content.

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://digitalfire.com, All Rights Reserved
Privacy Policy