1-9 | A | B | C | D | E | F | Frits | G | H | I | J | K | L | M | N | O | P | Q | R | S | T | U | V | W | X | Y | Z

Peerless 2 Kaolin

Alternate Names: Peerless China Clay, Peerless Kaolin

Description: Casting kaolin

Oxide Analysis Formula Tolerance
CaO 0.05% -
K2O 0.52% 0.01
MgO 0.07% -
Na2O 0.04% -
TiO2 1.40% 0.05
Al2O3 39.50% 1.00
SiO2 44.60% 1.92
Fe2O3 0.45% 0.01
LOI 13.30%n/a
Oxide Weight 223.70
Formula Weight 258.02

Notes

A large particle size kaolin of low plasticity. It is a secondary clay and has been mined since the 1940s. It is a moderately coarse grained clay that imparts more plasticity to a casting mix than similar clays produced by fractionation. It is used in sanitaryware, artware, generalware, floor tile, electrical porcelain, chemical porcelain and special refractories. In addition to improving casting properties, this material has excellent pressing properties.

This material is well crystallized with kaolinite being the predominant mineral. There is a trace of muscovite and less than 0.5% quartz.

Related Information

Links

Materials McNamee Kaolin
Materials Dixie Clay
Materials PAR Kaolin
Materials Langford Kaolin
Materials Bilt-Cote Kaolin
Materials Peerless 3 Kaolin
Materials Kaolin
The purest of all clays in nature. Kaolins are used in porcelains and stonewares to impart whiteness, in glazes to supply Al2O3 and to suspend slurries.
Typecodes Kaolin
Pure clay mineral, there are many brand names of varying purity and iron content.
URLs https://www.vanderbiltminerals.com/resources/Minerals_and_Chemical_for_Ceramics_and_Refractories_web.pdf
Vanderbilt Minerals for Ceramics Technical Sheet
Includes Vansil, Pyrax, Peerless, Dixie, Veegum, Vanzan, Darvan.

Data

Ultimate Particle Size Distribution -12 microns: 97% -5 microns: 78% -2.7 microns: 65% -1.0 microns: 52% -0.4 microns: 34%
Pyrometric Cone Equivalent Cone 34-35
Surface Area (m2/gm) 16.1
Median Particle Size (Microns) 1.1
pH for dry powder 4-6

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.