Description: Brick Clay Blend
| Oxide | Analysis | Formula | Tolerance |
|---|---|---|---|
| CaO | 0.20% | 0.02 | |
| K2O | 2.30% | 0.10 | |
| MgO | 0.40% | 0.04 | |
| Na2O | 0.40% | 0.03 | |
| TiO2 | 1.30% | 0.07 | |
| Al2O3 | 24.20% | 1.00 | |
| SiO2 | 63.20% | 4.43 | |
| Fe2O3 | 1.00% | 0.03 | |
| LOI | 7.00% | n/a | |
| C | 1.70% | n/a | |
| Oxide Weight | 391.98 | ||
| Formula Weight | 429.34 | ||
Particle Size (e.s.d.)
125 microns - 2.00
10 microns - 91
2 microns - 73
1 microns - 57
Modulus of Rupture at 110C
Mn/M2 - 7.6
lbf/in2 - 1110
Water Absorption
1120C - 2.5
1220C - 5.00
Shrinkage Dry to Fired
1120C - 8.50
1220C - 11.50
Refractoriness
Cone - 28, 1630C
| Typecodes |
Clay Other
Clays that are not kaolins, ball clays or bentonites. For example, stoneware clays are mixtures of all of the above plus quartz, feldspar, mica and other minerals. There are also many clays that have high plasticity like bentonite but are much different mineralogically. |
![]() PayPal | No tracking, No ads, No paywall, No transient content! Just organized, concise information constantly updated and improved. Was this helpful? Consider supporting me. |
| By Tony Hansen Follow me on ![]() | ![]() |
Buy me a coffee and we can talk