Pyrofrac 2024

Oxide Analysis Formula Tolerance
K2O 0.20% 0.01
Na2O 0.20% 0.02
TiO2 0.40% 0.03
Al2O3 19.60% 1.00
SiO2 73.80% 6.39
Fe2O3 1.00% 0.03
H2O 4.80%n/a
Oxide Weight 495.43
Formula Weight 520.41

Notes

Used in structural clay coatings, refractory formulations, whiteware ceramics, art pottery to
increase refractoriness, reduce shrinkage, and widen firing range.
This material is made by crushing & screening of selectively mined andalusite/pyrophyllite/sericite ores
with heavy media separation.

Related Information

Links

Materials Andalusite
A low expansion aluminum silicate mineral that converts to mullite on repeated firings.
Materials Pyrophyllite
A refractory aluminum silicate mineral often used in clay body recipes to lower thermal expansion, control fired maturity, mullite development catalyst, etc.
Materials Alkatrol
Materials Pyrofrac

Data

Bulk Density lbs/cu. ft. (Packed) 70
Pyrometric Cone Equivalent 27
Sieve Analysis Dry +20 mesh: 10.1 +50 mesh: 59.3 +70 mesh: 13.5 +100 mesh: 8.2 +200 mesh: 7.0 +325 mesh: 1.0
Density (Specific Gravity) 2.7

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://digitalfire.com, All Rights Reserved
Privacy Policy