Pemco Frit P-2201

Alternate Names: Frit 2201, Frit P2201

Description: Calcium borate frit, Gerstley Borate substitute

Oxide Analysis Formula Tolerance
CaO 22.20% 0.63
MgO 4.80% 0.19
Na2O 6.80% 0.18
B2O3 51.50% 1.18
Al2O3 1.50% 0.02
SiO2 13.20% 0.35
Oxide Weight 160.13
Formula Weight 160.13

Related Information

Links

Materials Fusion Frit F-309
Materials Frit
Frits are made by melting mixes of raw materials, quenching the melt in water, grinding the pebbles into a powder. Frits have chemistries raw materials cannot.
Typecodes Frit
A frit is the powdered form a man-made glass. Frits are premelted, then ground to a glass. They have tightly controlled chemistries, they are available for glazes of all types.

Data

Co-efficient of Linear Expansion 8.40
Co-efficient of Linear Expansion 8.40 (50-450C)
Frit Softening Point 1370F
Frit Melting Range (C) 1320-1420F
I.F.P. (celsius) 621C

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://digitalfire.com, All Rights Reserved
Privacy Policy