Alternate Names: Fusion Frit FZ565
Description: CaZn frit for slow fire
| Oxide | Analysis | Formula | Tolerance |
|---|---|---|---|
| Al2O3 | 8.50% | 0.17 | |
| MgO | 0.50% | 0.03 | |
| ZnO | 11.20% | 0.28 | |
| CaO | 13.50% | 0.49 | |
| Na2O | 5.80% | 0.19 | |
| K2O | 0.50% | 0.01 | |
| B2O3 | 1.50% | 0.04 | |
| SiO2 | 58.50% | 1.99 | |
| Oxide Weight | 204.29 | ||
| Formula Weight | 204.29 | ||
| URLs |
http://www.fusionceramics.com/
Fusion Ceramics Frit Website |
| Typecodes |
Frit
A frit is the powdered form a man-made glass. Frits are premelted, then ground to a glass. They have tightly controlled chemistries, they are available for glazes of all types. |
| Co-efficient of Linear Expansion | 7.78 x 10-6 |
|---|---|
| Frit Softening Point | 1550F |