Fusion Frit F-10

Alternate Names: Fusion Frit F10

Description: Opacified flux for cone 1 tile glazes

Oxide Analysis Formula Tolerance
CaO 2.50% 0.14
K2O 5.50% 0.18
Na2O 13.50% 0.68
ZrO2 13.00% 0.33
B2O3 12.00% 0.54
Al2O3 8.50% 0.26
SiO2 45.00% 2.33
Oxide Weight 311.83
Formula Weight 311.83

Related Information

Links

Materials Frit
Frits are made by melting mixes of raw materials, quenching the melt in water, grinding the pebbles into a powder. Frits have chemistries raw materials cannot.
URLs http://www.fusionceramics.com/
Fusion Ceramics Frit Website
Typecodes Frit
A frit is the powdered form a man-made glass. Frits are premelted, then ground to a glass. They have tightly controlled chemistries, they are available for glazes of all types.

Data

Co-efficient of Linear Expansion 8.74 x 10-6
Frit Softening Point 1600F

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://digitalfire.com, All Rights Reserved
Privacy Policy