Frit A 3069

Alternate Names: Frit A3069, Frit 3069P, Fritte3069P

Description: Reimbold & Strick low expansion Li frit

Oxide Analysis Formula Tolerance
Li2O 2.00% 0.47
MgO 3.00% 0.53
Al2O3 9.00% 0.62
SiO2 57.00% 6.70
B2O3 29.00% 2.94
Oxide Weight 706.44
Formula Weight 706.44

Related Information

Links

Materials Frit
Frits are made by melting mixes of raw materials, quenching the melt in water, grinding the pebbles into a powder. Frits have chemistries raw materials cannot.
Typecodes Frit
A frit is the powdered form a man-made glass. Frits are premelted, then ground to a glass. They have tightly controlled chemistries, they are available for glazes of all types.

Data

Co-efficient of Linear Expansion 40 x 10-7 (20-400C)
Frit Softening Point 640C
Glass Transition Temperature 540C

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://digitalfire.com, All Rights Reserved
Privacy Policy