Description: High zinc opacified frit
| Oxide | Analysis | Formula | Tolerance |
|---|---|---|---|
| ZnO | 11.43% | 0.34 | |
| Al2O3 | 6.99% | 0.17 | |
| ZrO2 | 9.78% | 0.19 | |
| MgO | 2.35% | 0.14 | |
| Na2O | 0.56% | 0.02 | |
| SiO2 | 55.40% | 2.24 | |
| K2O | 4.02% | 0.10 | |
| Fe2O3 | 0.13% | - | |
| CaO | 9.05% | 0.39 | |
| TiO2 | 0.08% | - | |
| LOI | 0.11% | n/a | |
| Oxide Weight | 242.35 | ||
| Formula Weight | 242.62 | ||
| Typecodes |
Frit
A frit is the powdered form a man-made glass. Frits are premelted, then ground to a glass. They have tightly controlled chemistries, they are available for glazes of all types. |