C-B Clay

Alternate Names: Spinks C-B, C-B Ball Clay

Description: Ball Clay

Oxide Analysis Formula Tolerance
CaO 0.26% 0.02
K2O 0.84% 0.03
MgO 0.23% 0.02
Na2O 0.22% 0.01
TiO2 1.50% 0.07
Al2O3 26.42% 1.00
P2O5 0.12% -
SiO2 57.78% 3.71
Fe2O3 0.98% 0.02
MnO 0.02% -
LOI 11.59%n/a
SO3 0.06%n/a
Oxide Weight 341.17
Formula Weight 386.16

Notes

Relative Viscosity (1.2 Sp. Gr.):* 1.47
Casting Rate: (gms per 15 min/426 cm2):* 190
Water of Plasticity:* 20.2
% Dry Shrinkage:* 4.86
Dry M.O.R., psi:* 700

Cone 04 8 11
----
Fired Shrinkage:* 0.1% 1.0% 1.9%
Absorption:* 18.2% 16.9% 15.0%
M.O.R. psi:* 1600 3159 3497

Thermal Expansion, Cone 8: 0.48% at 700C
P.C.E.: 32
pH: 4.6
Oil Absorption: 35
Bulk Density, lbs per cubic foot: 35-40
Particle Size, Microns: 20 10 5 2 1 0.5 0.2
96% 88% 77% 60% 45% 27% 10%

*Specimens: De-aired, extruded, 50% ball clay, 50% flint

Related Information

Links

Typecodes Ball Clay
Ball clays are abundant and very plastic and are used in all types of plastic forming bodies. They are not as white-burning or refractory as kaolins but lower in iron and fluxes than bentonites.

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://digitalfire.com, All Rights Reserved
Privacy Policy