Layton Clay

Alternate Names: Layton Kaolin

Oxide Analysis Formula Tolerance
CaO 0.25% 0.01
K2O 0.11% -
MgO 0.24% 0.02
Na2O 0.30% 0.01
TiO2 1.29% 0.04
Al2O3 37.07% 1.00
SiO2 46.55% 2.13
Fe2O3 0.66% 0.01
LOI 13.53%n/a
Oxide Weight 237.93
Formula Weight 275.16

Related Information

Links

Materials Kaolin
The purest of all clays in nature. Kaolins are used in porcelains and stonewares to impart whiteness, in glazes to supply Al2O3 and to suspend slurries.
Typecodes Clay Other
Clays that are not kaolins, ball clays or bentonites. For example, stoneware clays are mixtures of all of the above plus quartz, feldspar, mica and other minerals. There are also many clays that have high plasticity like bentonite but are much different mineralogically.

Data

% < 0.5 microns 25%
Firing Shrinkage 17% at cone 9
Water absorption 7% at cone 9
Dry M.O.R. (50% Silica) 950

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://digitalfire.com, All Rights Reserved
Privacy Policy