Oct 22, 2026: We are working on protecting our servers against the PHP2Shell vulnerability recently discovered. Servers were upgraded ahead of schedule on Oct 21. This could cause some issues. Please contact us if you encounter any.

1-9 | A | B | C | D | E | F | Frits | G | H | I | J | K | L | M | N | O | P | Q | R | S | T | U | V | W | X | Y | Z

Kaiser Missouri Fireclay

Oxide Analysis Formula Tolerance
CaO 0.28% 0.02
K2O 0.70% 0.02
MgO 0.22% 0.02
Na2O 0.71% 0.04
TiO2 1.35% 0.06
Al2O3 30.44% 1.00
SiO2 53.45% 2.98
Fe2O3 1.61% 0.03
LOI 11.23%n/a
Oxide Weight 297.42
Formula Weight 335.05

Notes

Kaiser was reorganized into National refractories in 1985, the fireclay is now sold at NAT Dry Milled Fireclay.

Related Information

Links

Materials NAT Dry Milled Fireclay
Materials Fireclay
Typecodes Fireclay
Fireclays are non-kaolin non-ball clay materials similar to stoneware clays but lacking fluxing oxides. Many fireclays have a PCE of 28 or more.

Data

Pyrometric Cone Equivalent 31

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://digitalfire.com, All Rights Reserved
Privacy Policy