G-40 Feldspar

Description: Potash/sodium/calcium Feldspar

Oxide Analysis Formula Tolerance
CaO 0.80% 0.08
MgO 0.05% 0.01
K2O 10.40% 0.63
Na2O 3.00% 0.28
Al2O3 18.00% 1.01
SiO2 67.56% 6.45
Fe2O3 0.08% -
LOI 0.16%n/a
Oxide Weight 573.12
Formula Weight 574.04

Notes

G-40 is a potassium / sodium / calcium aluminum silicate used as a source of alumina and potash in specialized glass batch formulations requiring higher potassium levels. Carefully beneficiated using the froth flotation process, G-40 Feldspar offers low iron oxide and high alkali oxide content per unit of alumina.

Related Information

Links

URLs http://www.zemex.com/feldspar/g40spar.html
G40 Data Sheet
Materials G-20 Feldspar
Materials Potash Feldspar
A feldspar having a KNaO content that predominates in potassium.
Typecodes Feldspar
The most common source of fluxes for high and medium temperature glazes and bodies.

Data

Bulk Density lbs/cu. ft. (Packed) 90
Sieve Analysis Dry +30 mesh: tr +40 mesh: 0.3 +200 mesh: 94.8

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://digitalfire.com, All Rights Reserved
Privacy Policy