28 Clay

Description: Plastic Clay - Allier, France

Oxide Analysis Formula Tolerance
CaO 0.20% 0.02
K2O 1.40% 0.07
MgO 0.20% 0.02
Na2O 0.10% 0.01
TiO2 1.90% 0.11
Al2O3 21.50% 1.00
SiO2 66.20% 5.23
Fe2O3 1.40% 0.04
LOI 7.10%n/a
C 0.30%n/a
Oxide Weight 440.73
Formula Weight 475.96

Notes

Raw Color - Light Cream - Cream
Particle Size (e.s.d.)
125 microns - 1.0
63 microns - 4.0
20 microns - 92
2 microns - 54
.5 microns - 18
Modulus of Rupture at 110C
Mn/M2 - 2.9
lbf/in2 - 430
Water Absorption
1120C - 13.0
1220C - 5.50
Shrinkage Dry to Fired
1120C - 5.0
1220C - 10.0
Refractoriness
Cone - , 1750C
Plastic Index - 841
PF NO. - 36.2

Related Information

Links

Typecodes Clay Other
Clays that are not kaolins, ball clays or bentonites. For example, stoneware clays are mixtures of all of the above plus quartz, feldspar, mica and other minerals. There are also many clays that have high plasticity like bentonite but are much different mineralogically.

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://digitalfire.com, All Rights Reserved
Privacy Policy