Digitalfire is facing a takedown order from Plainsman Clays. They are revoking permission to "use any Plainsman content" "on any platform". This is broad and vague enough, and this site large enough, that I am unable to comply or even interpret it in the short timeframe (June 27). Please don't panic, I am overwhelmed by the unbelievable support I am getting. We just need to get them to relent on this demand and call off the lawyer (to at least permit commentary). There are lots of backup sites (many people have the API endpoints), don't start downloading or scraping again and overload the server.

Insight-live.com general operation is not affected by this.

1-9 | A | B | C | D | E | F | Frits | G | H | I | J | K | L | M | N | O | P | Q | R | S | T | U | V | W | X | Y | Z

FT-YC Clay

Description: Westerwald, Germany - Plastic Clay

Oxide Analysis Formula Tolerance
CaO 0.20% 0.02
K2O 1.20% 0.06
MgO 0.20% 0.02
Na2O 0.20% 0.02
TiO2 2.00% 0.12
Al2O3 21.40% 1.00
SiO2 65.50% 5.19
Fe2O3 2.00% 0.06
LOI 7.30%n/a
C 0.30%n/a
Oxide Weight 441.84
Formula Weight 478.18

Notes

Raw Color - YELLOW
Particle Size (e.s.d.)
125 microns - 2.6
63 microns - 6.3
20 microns - 89
2 microns - 70
.5 microns - 56
Modulus of Rupture at 110C
Mn/M2 - 5.6
lbf/in2 - 810
Water Absorption
1120C - 5.0
1220C - 1.00
Shrinkage Dry to Fired
1120C - 5.0
1220C - 6.0
Plastic Index - 650
PF NO. - 31.0

Related Information

Links

Typecodes Clay Other
Clays that are not kaolins, ball clays or bentonites. For example, stoneware clays are mixtures of all of the above plus quartz, feldspar, mica and other minerals. There are also many clays that have high plasticity like bentonite but are much different mineralogically.

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://digitalfire.com, All Rights Reserved
Privacy Policy