1-9 | A | B | C | D | E | F | Frits | G | H | I | J | K | L | M | N | O | P | Q | R | S | T | U | V | W | X | Y | Z

FT-201 Clay

Description: Westerwald, Germany - Plastic Clay

Oxide Analysis Formula Tolerance
CaO 0.20% 0.03
K2O 1.50% 0.12
MgO 0.30% 0.05
Na2O 0.20% 0.02
TiO2 1.30% 0.12
Al2O3 13.90% 1.00
SiO2 76.60% 9.35
Fe2O3 2.10% 0.10
LOI 4.00%n/a
C 0.30%n/a
Oxide Weight 705.19
Formula Weight 736.88

Notes

Raw Color - CREAM
Particle Size (e.s.d.)
125 microns - 0.5
63 microns - 8.0
20 microns - 82
2 microns - 47
.5 microns - 35
Modulus of Rupture at 110C
Mn/M2 - 3.6
lbf/in2 - 530
Water Absorption
1120C - 0.5
1220C - 2.00
Shrinkage Dry to Fired
1120C - 2.0
1220C - 4.3
Refractoriness
Cone - 28, 1630C
Plastic Index - 500
PF NO. - 24.0

Related Information

Links

Typecodes Clay Other
Clays that are not kaolins, ball clays or bentonites. For example, stoneware clays are mixtures of all of the above plus quartz, feldspar, mica and other minerals. There are also many clays that have high plasticity like bentonite but are much different mineralogically.