Pemco Frit P-1701

Alternate Names: Frit 1701, Frit P1701

Description: LEADLESS FRIT

Oxide Analysis Formula Tolerance
CaO 4.70% 0.46
K2O 1.00% 0.06
Li2O 0.40% 0.07
Na2O 3.90% 0.35
SrO 1.10% 0.06
B2O3 27.00% 2.14
Al2O3 9.10% 0.49
SiO2 52.80% 4.84
Oxide Weight 551.45
Formula Weight 551.45

Notes

All-fritted glaze for high alumina bodies firing in the range of 1600-1800F.

Related Information

Links

Materials Frit
Frits are made by melting mixes of raw materials, quenching the melt in water, grinding the pebbles into a powder. Frits have chemistries raw materials cannot.
Materials Fusion Frit F-79
Materials Hommel Frit 487
Typecodes Frit
A frit is the powdered form a man-made glass. Frits are premelted, then ground to a glass. They have tightly controlled chemistries, they are available for glazes of all types.

Data

Co-efficient of Linear Expansion 5.40
Co-efficient of Linear Expansion 5.40 (50-450C)
Frit Softening Point 1490F
Frit Melting Range (C) 1460-1550F
I.F.P. (celsius) 612C

PayPal
No tracking, No ads, No paywall, No transient content!
Just organized, concise information constantly updated and improved.
Was this helpful? Consider supporting me.
By Tony Hansen
Follow me on

Got a Question?

Buy me a coffee and we can talk

 



https://digitalfire.com, All Rights Reserved
Privacy Policy