Alternate Names: GIMMica CD-3200
| Oxide | Analysis | Formula | Tolerance |
|---|---|---|---|
| SiO2 | 48.30% | 2.23 | |
| Al2O3 | 36.70% | 1.00 | |
| K2O | 4.25% | 0.13 | |
| Fe2O3 | 0.69% | 0.01 | |
| MgO | 0.12% | 0.01 | |
| Na2O | 0.21% | 0.01 | |
| TiO2 | 0.35% | 0.01 | |
| LOI | 8.00% | n/a | |
| Oxide Weight | 251.86 | ||
| Formula Weight | 273.76 | ||
CD-3200 is a water ground muscovite mica that has optimum delamination and high purity. Our patented process produces a mica product that gives optimum performance in a variety of applications. In addition to excellent color, CD-3200 creates a functional pigment that is very desirable where low bulk density, fineness, high aspect ratio, and excellent coverage are required.
Performance Characteristics
The performance characteristics that make
CD-3200 an acceptable cost effective additive for these markets are:
Excellent color
Ease of dispersion
Increased coverage
Chemical inertness
Superior barrier properties
High temperature stability
Superior dielectric properties
Superior reinforcement properties
Mean Particle Size, microns 15 - 25 18
Sieve Analysis, % retained
+100 mesh Trace Trace
+200 mesh 1.0 max. 0.8
+325 mesh 4 - 12 6
Bulk Density (Colgate method) 8 - 14 12
Moisture Loss, 100Cº, % <0.5
Color, L value >90
Mineral Muscovite mica
Chemical Composition Potassium aluminum silicate
Specific gravity 2.82
CAS# 12001-26-2
ph 6.0 - 7.5
| URLs |
http://www.gimmica.com/
Company website |
| Materials |
Mica
|
| Typecodes |
Aluminum Silicate
Materials not classifiable as commonly known aluminum silicates. For example, kaolin is a common aluminum silicate. |
![]() PayPal | No tracking, No ads, No paywall, No transient content! Just organized, concise information constantly updated and improved. Was this helpful? Consider supporting me. |
| By Tony Hansen Follow me on ![]() | ![]() |
Buy me a coffee and we can talk