| Oxide | Analysis | Formula | Tolerance |
|---|---|---|---|
| CaO | 0.02% | 0.08 | |
| K2O | 0.08% | 0.19 | |
| TiO2 | 0.01% | 0.03 | |
| Al2O3 | 0.45% | 1.00 | |
| SiO2 | 99.20% | 374.13 | |
| Fe2O3 | 0.03% | 0.04 | |
| LOI | 0.20% | n/a | |
| Oxide Weight | 22,619.07 | ||
| Formula Weight | 22,664.40 | ||
| Minerals |
Quartz
Quartz is the most abundant mineral on earth, it is the main crystalline mineral form of silica (SiO |
| Typecodes |
Silica/Quartz
Quartz is very abundant and there are many grades and name brands. |
| Bulk Density g/cc (Packed) | 1.2 |
|---|---|
| Hardness (Moh) | 7 |
| Ultimate Particle Size Distribution | >30 micron: 1.5% |
| Density (Specific Gravity) | 2.6 |
| pH for dry powder | 8-9 |
![]() PayPal | No tracking, No ads, No paywall, No transient content! Just organized, concise information constantly updated and improved. Was this helpful? Consider supporting me. |
| By Tony Hansen Follow me on ![]() | ![]() |
Buy me a coffee and we can talk